In the automobile coating process, the top coat is the last process of Z. with the continuous development of the automobile industry, many manufacturers now use baking paint. If there is a problem after finishing, it is Z troublesome. The following atomic ash manufacturers will make a brief introduction according to the problems in production.
 
1. The top coat foams after baking.
 
Scrape off the bubbles after the bubbles of the top coat and see which layer the bubbles are on. If the bubbles appear in the primer layer, the atomic ash is well combined with the primer, and the substrate treatment may not be in place; After blowing off the bubbles, it is found that there is a layer of primer on the atomic ash and the substrate. Then it may be that the primer is too thick or the primer is not dry enough.
 
2. Pinholes and depressions appear after baking the finish paint.
 
First of all, consider whether the pinhole has its own quality. Secondly, if pinholes appear when the quality of atomic ash is qualified, it is generally because the atomic ash coating and grinding technology is poor and the sand holes are not handled well. In addition, during the coating and scraping process, if the coating and scraping tool is improperly selected, it will also cause pinholes.
 
3. "Prickle" after baking the finish coat.
 
First, the climate is too humid and the water absorption of the atomic ash is too large. The polished atomic ash adsorbs a considerable amount of water. The topcoat is sprayed before the water volatilizes. A small amount of water is sealed under the paint film. Once heated, the water volume expands sharply and breaks through the paint film to form a "prickly heat". Second, the water absorption of atomic ash is qualified. After being dried by hot air, spray the top coat, and there is "prickly heat" after baking. Then it is possible that after spraying the top coat, the solvent enters the drying room before it volatilizes fully. In this way, because the surface of the top coat is closed soon, the residual solvent has to break through the paint film to form "prickly heat". Of course, it may also be the quality problem of the topcoat, or the mismatch between the polarity of the solvent and the topcoat


Prev What are the types of atomic ash
NextSteps for scraping atomic ash

Copyright © 2020 Changxing Baodi Environmental Protection Technology Co., Ltd all reserved Web Admin --> >>

浙公網安備 33052202000243號?浙ICP備17019658號

主站蜘蛛池模板: 72pao成人国产永久免费视频 | 欧美一区二区精品夜夜嗨 | 在线香蕉视频 | 日本精品一区二区 | 国产精品久久久久久婷婷天堂 | 中国av免费在线观看 | 99精彩视频在线观看 | 精品国产一区二区三区四区在线 | 午夜在线观看视频网站 | 成人在线视频在线观看 | 超碰九色| 免费观看黄色一级视频 | 亚洲一区二区三区视频免费 | 色天天综合网 | 日韩中文字幕三区 | 成人免费一区二区三区 | 国产精品久久久久久影院8一贰佰 | 黄色一级片在线免费观看 | 国产乱淫av | 欧美女同hd | 蜜桃av网| 9丨九色丨国产 | 性大片性大片免费 | 免费a级毛片大学生免费观看 | 欧美18—19sex性hd按摩 | 欧美黄成人免费网站大全 | 国产精品久久久久久238 | 91看片在线观看视频 | 操操电影| 亚洲精品动漫在线观看 | 黄色网址在线播放 | 中国一级毛片在线视频 | 日韩视频―中文字幕 | 欧美一区二区三区免费不卡 | 草草视频免费 | 羞羞羞网站 | 亚洲人成中文字幕在线观看 | 国产亚洲综合一区二区 | 韩国十九禁高潮床戏在线观看 | 久久在线| 艹男人的日日夜夜 |